In this work, we present magnetic and electrical properties of La0.67Ca0.33Mn1−xVxO3 (x=0x=0 and 0.1). Polycrystalline La0.67Ca0.33MnO3 and La0.67Ca0.33Mn0.9V0.1O3 samples were prepared by conventional solid-state reaction. Two Curie temperatures for the La0.67Ca0.33Mn0.9V0.1O3 sample were observed at Tc1=223K and Tc2=190K. The undoped La0.67Ca0.33MnO3 sample showed only one magnetic transition temperature at 267 K. The temperature dependence of resistance showed two maxima in the V-doped sample, and the peak value of magnetoresistance (MR) around the Curie temperature increased with V doping. Double maxima in the resistance–temperature and magnetisation–temperature curves are explained by the existence of two phases in La0.67Ca0.33Mn0.9V0.1O3 samples.
Journal: Physica B: Condensed Matter - Volume 371, Issue 2, 31 January 2006, Pages 199–204